PC Blow Molding Bottle Material Control Essentials (Extrusion Blow Molding)
PC is an amorphous, high-viscosity, strongly hygroscopic material with a narrow melt-strength window. The essence of material control comes down to two things: prevent hydrolysis/degradation + stabilize melt strength, and control sag and internal stress.
Key point: PC viscosity is extremely sensitive to temperature; once moisture exceeds the limit, high-temperature hydrolysis breaks the molecular chains and melt strength collapses — no amount of temperature adjustment can save it.
I. Resin & Drying (Top Priority — the Foundation of Material Control)
- Grade selection: Must use blow-molding-grade PC (high molecular weight). Ordinary injection-molding PC lacks melt strength, causing severe parison sag; keep regrind ratio ≤20% (too much regrind lowers melt strength and causes brittleness), and dry regrind separately.
- Drying standard (dehumidifying dryer, dew point ≤ -40°C; ordinary hot-air drying is not acceptable):
- Temperature: 120°C
- Time: 4–6 h; thick-walled bottles / regrind: extend to 6–8 h
- Target moisture: ≤0.02% (200 ppm); for high-transparency, stress-resistant grades keep within 0.015%
- After drying, maintain hopper temperature at ~110°C; dried material exposed to air for more than half an hour must be re-dried.
- Diagnosis: silver streaks, bubbles, soft sagging parison, brittle bottles, poor impact — first check moisture.
II. Temperature Profile (Determines Melt Viscosity, Melt Strength, Degradation)
Recommended extrusion-blow temperature range (accumulator head):
- Barrel rear (feed zone): 260–270°C
- Middle zone: 280–290°C
- Front zone / adapter: 290–300°C
- Die head: 285–295°C (slightly lower than the front zone, to preserve melt strength)
- Upper limit red line: Do not exceed 310°C for extended periods — prolonged residence causes yellowing, black specks, and molecular degradation.
Tuning logic:
- Temperature too high: viscosity thins, melt strength ↓ → parison sags and stretches, thick bottom / thin top, easy to blow out, yellowing
- Temperature too low: viscosity too high, large die swell, unstable output, poor weld-line quality, surging internal stress, later cracking
- PC has a narrow tuning window — adjust only ±3–5°C per trial; do not make large changes.
III. Plastication & Shear Control (Screw Speed, Back Pressure, Residence Time)
- Screw speed: keep low — low-speed plastication reduces shear heat; high speed = shear heat spikes, causing localized over-temperature degradation.
- Back pressure: medium-low, enough to ensure uniform plastication and degassing; too high = excessive shear, breaking molecular chains, making the material brittle.
- Residence time: PC must not sit in the barrel/accumulator for too long; if stopped for more than 20 minutes, lower the temperature, purge, or clean. Die-head channels must be streamlined with no dead corners where material can accumulate and carbonize.
IV. Parison Properties (Melt Strength + Sag Control — the Hardest Part of PC Blow Molding)
PC melt strength is much lower than PE, so self-weight sag is the norm:
- Parison temperature uniformity comes first — large circumferential temperature differences cause one side to sag while the other doesn't, leading to uneven wall thickness.
- The wall thickness controller (PWG) must enable sag compensation: program the upper section with increased output to compensate for thinning, and narrow the gap in the lower section.
- Practical approach: for the same resin, to improve melt strength and resist sag: lower die-head temperature by 5°C + moderately increase extrusion speed to shorten parison hang time.
- Blow-up ratio: keep to 1.8–2.5. Blowing too large over-orients the molecular chains, causing high internal stress, whitening of transparent parts, and susceptibility to solvent cracking.
V. Mold Temperature & Cooling (Directly Determines Internal Stress)
PC's biggest common problem: internal stress cracking (cracks easily when filled with alcohol, cleaning agents, fragrances).
- Mold temperature: for extrusion-blow PC, oil temperature 90–110°C (prefer ~100°C).
- Mold too cold: quench cooling — molecular chains have no time to relax, huge internal stress, hazy appearance, poor transparency, later stress cracking.
- Mold too hot: longer cooling cycle, soft deformation on demolding, slower production.
- Cooling: uniform, gradient cooling; slow cooling at thick sections (bottom, shoulder); highly stress-resistant bottles can add an annealing step (hold at 110°C for tens of minutes, slow cool).
- Blow air pressure: 0.4–0.8 MPa; pre-blow is critical — pre-blow too early easily blows through the soft parison; pre-blow too late and the sag is already set, wall thickness can't be recovered.
VI. Quick Material-Anomaly Diagnosis Table
表格
| Symptom | Material Root Cause | Priority Adjustment |
|---|---|---|
| Silver streaks, bubbles | Excess moisture, hydrolysis | Check dryer dew point, re-dry |
| Parison keeps stretching down, thick bottom / thin top | Insufficient melt strength (high temp / hydrolysis / wrong grade) | Lower die-head temp, shorten hang time, check moisture |
| Bottle transparent but cracks on solvent contact | High internal stress | Raise mold temp, slow cooling, reduce blow-up ratio |
| Yellowing, black specks | Local over-temperature, degraded accumulated material | Lower temp, clean die-head dead corners, reduce residence |
| Parison surface pitting, orange peel | Uneven plastication, low temperature, poor degassing | Slightly raise melt temp, check die-head venting |
| Bottle brittle, dropped bottom | Molecular degradation (water + high temp + strong shear) | Control moisture first, then lower screw speed and back pressure |
VII. Practical Tuning Sequence (Recommended Order)
- Confirm the resin is blow-molding grade, regrind ratio is compliant, and material is fully dried.
- Stabilize the drying system first — only run once the dew point passes.
- Set the base temperature profile, run a low-speed air purge, and check whether the parison is clear with no silver streaks and uniform circumferential output.
- Observe parison sag; fine-tune die-head temperature + wall-thickness compensation program.
- Adjust mold temperature (prioritize raising it to control stress), pre-blow timing, and blow air pressure.
- Stress-test finished bottles (immerse in solvent to check for cracking), then refine further.